Nargusta

Nargusta (Terminalia amazonia)
Nargusta (Terminalia amazonia)

View More Images Below

Common Name(s): Nargusta, Canxan Negro

Scientific Name: Terminalia amazonia

Distribution: From Mexico to Brazil

Tree Size: 100-165 ft (30-50 m) tall, 3-5 ft (1-1.5 m) trunk diameter

Average Dried Weight: 49 lbs/ft3 (785 kg/m3)

Specific Gravity (Basic, 12% MC): .66, .79

Janka Hardness: 1,750 lbf (7,770 N)

Modulus of Rupture: 17,770 lbf/in2 (122.5 MPa)

Elastic Modulus: 2,205,000 lbf/in2 (15.21 GPa)

Crushing Strength: 9,570 lbf/in2 (66.0 MPa)

Shrinkage: Radial: 6.4%, Tangential: 8.7%, Volumetric: 14.9%, T/R Ratio: 1.4

Color/Appearance: Heartwood varies from light to medium brown, sometimes with a golden or olive cast. Occasionally seen with darker reddish brown streaks. The yellow sapwood is not easily distinguished from heartwood.

Grain/Texture: Grain is usually interlocked, but can sometimes be straight grained. With a fine, uniform texture, and good natural luster.

Endgrain: No data available.

Rot Resistance: Varies from very durable to moderately durable; mixed insect resistance.

Workability: Can be difficult to work due to interlocked grain, resulting in tearout. Wood with straight grain has better working characteristics. Glues and finishes well.

Odor: No characteristic odor.

Allergies/Toxicity: Although there have been no adverse health effects associated with Nargusta, a number of other related species within the Terminalia genus have been reported to cause skin irritation. See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Pricing/Availability: Seldom exported in lumber form, Nargusta is usually only available as smaller craft lumber and turning blanks, particularly sections of burl wood. Expect prices to be in the mid range for an imported hardwood.

Sustainability: This wood species is not listed in the CITES Appendices or on the IUCN Red List of Threatened Species.

Common Uses: Turned objects, furniture, cabinetry, boatbuilding, and general construction.

Comments: No data available.

Related Species:

Related Articles:

None available.

Scans/Pictures: Samples scanned are from burl wood, and do not represent regular lumber.

Nargusta (Terminalia amazonia)
Nargusta (sanded)
Nargusta (sealed)
Nargusta (sealed)
   